Specification of Portland Blast Furnace Slag Cement European Standard EN 197-1/2000

CHEMICAL COMPOSITIONS

CHEMICAL COMPOSITIONS
LIMITS AS EN 197-1/2000
TIGER CEMENT TEST RESULTS
L.O.INot more than 4.0%1.86
SiO2Not Specified22.19
AI2O3Not Specified4.88
Fe2O3Not Specified3.86
CaONot Specified60.61
MgONot more than 7.0%2.55
SO3Not more than 3.0%1.77
T. AlkaliesNot Specified0.48
I.R.Not more than 1.50%0.72

PHYSICAL TEST

PHYSICAL TEST
LIMITS AS PER EN 197-1/2000
TIGER CEMENT TEST RESULTS
Residue 1702Not more than 10.0%5.4
Blaine (cm2/gm)Not less than 22502958
Setting time
InitialNot less than 75 minutes195
FinalNot more than 600 minutes220
Soundness ExpansionNot more than 10.0 minutesNil
Compressive strengths
03 DaysNot less than 2200 PSI3216
07 DaysNot less than 3400 PSI4160
28 DaysNot less than 5000 PSI5730
L.S.FNot < 0.66 & Not > 1.020.85
S MNot Specified2.54
AMNot Specified1.26